| Typical Properties |
|
Heat Treat State |
Typical |
|
Coefficient of Thermal Expansion (per F @ 68-212F)
|
|
12.4
|
|
Coefficient of Thermal Expansion (per F @ 68-572F)
|
|
13.7
|
|
Melting Range (Liquidus-Solidus)(F)
|
|
1015-1150
|
|
Resistance to Hot Cracking
|
|
E
|
|
Pressure Tightness
|
|
E
|
|
Fluidity
|
|
E
|
|
Solidification Shrinkage Tendency
|
|
E
|
|
Strength at Elevated Temperatures
|
|
VG
|
|
Corrosion Resistance
|
|
G
|
|
Machinability
|
|
G
|
|
Polishing
|
|
G
|
|
Gas Welding
|
|
E
|
|
Arc Welding
|
|
E
|
|
Brazing
|
|
No
|
|
Normally Heat Treated
|
|
Yes
|
|
Annodizing Appearance
|
|
Gray
|
|
Electroplating
|
|
VG
|
|
Compressive Yield Strength (ksi)
|
T51
|
24
|
|
Hardness (Brinell) (HB @ 500kg)
|
T51
|
65
|
|
Shear Strength (ksi)
|
T51
|
22
|
|
Endurance Limit (K ksi)
|
T51
|
8
|
|
Electrical Conductivity (% IACS @ 68F)
|
T51
|
43
|
|
Thermal Conductivity (cal/sec/sq cm/cm/C @ 25C)
|
T51
|
0.4
|
|
Compressive Yield Strength (ksi)
|
T6
|
26
|
|
Hardness (Brinell) (HB @ 500kg)
|
T6
|
80
|
|
Shear Strength (ksi)
|
T6
|
28
|
|
Endurance Limit (K ksi)
|
T6
|
9
|
|
Electrical Conductivity (% IACS @ 68F)
|
T6
|
36
|
|
Thermal Conductivity (cal/sec/sq cm/cm/C @ 25C)
|
T6
|
0.34
|
|
Compressive Yield Strength (ksi)
|
T7
|
38
|
|
Hardness (Brinell) (HB @ 500kg)
|
T7
|
85
|
|
Shear Strength (ksi)
|
T7
|
28
|
|
Endurance Limit (K ksi)
|
T7
|
10
|
|
Electrical Conductivity (% IACS @ 68F)
|
T7
|
42
|
|
Thermal Conductivity (cal/sec/sq cm/cm/C @ 25C)
|
T7
|
0.39
|
|
Compressive Yield Strength (ksi)
|
T71
|
30
|
|
Hardness (Brinell) (HB @ 500kg)
|
T71
|
75
|
|
Shear Strength (ksi)
|
T71
|
26
|
|
Endurance Limit (K ksi)
|
T71
|
10
|
|
Modulus of Elasticity (K ksi)
|
T71
|
10.2
|
|
Electrical Conductivity (% IACS @ 68F)
|
T71
|
39
|
|
Thermal Conductivity (cal/sec/sq cm/cm/C @ 25C)
|
T71
|
0.36
|