Typical Properties |
|
Heat Treat State |
Typical |
Compressive Yield Strength (ksi)
|
|
38
|
Shear Strength (ksi)
|
|
40
|
Density (lb/cu.in. @ 68F)
|
|
.101
|
Electrical Conductivity (% IACS @ 68F)
|
|
30
|
Thermal Conductivity (cal/sec/sq cm/cm/C @ 25C)
|
|
0.29
|
Coefficient of Thermal Expansion (per F @ 68-212F)
|
|
10.7
|
Melting Range (Liquidus-Solidus)(F)
|
|
1058-1202
|
Resistance to Hot Cracking
|
|
F
|
Pressure Tightness
|
|
G
|
Fluidity
|
|
G
|
Solidification Shrinkage Tendency
|
|
F
|
Strength at Elevated Temperatures
|
|
E
|
Corrosion Resistance
|
|
F
|
Machinability
|
|
E
|
Polishing
|
|
E
|
Gas Welding
|
|
F
|
Arc Welding
|
|
F
|
Normally Heat Treated
|
|
Yes
|
Annodizing Appearance
|
|
VG
|
Electroplating
|
|
E
|